Polyester-based Thermoplastic Polyurethane
| Properties | Key | NORM | Value | Unit |
|---|---|---|---|---|
| Hardness (after 3 sec.) | M | ISO 7619 | 68 | Shore A |
| Density | M | ISO 1183-1 | 1.17 | g/cm³ |
| Tensile strength | M | DIN 53504 | 45 | MPa |
| Elongation @ break | M | DIN 53504 | 700 | % |
| Tensile stress @ 100% elongation | M | DIN 53504 | 3.2 | MPa |
| Tensile stress @ 300% elongation | M | DIN 53504 | 7.8 | MPa |
| Tear strength | M | ISO 34-1 | 50 | N/mm |
| Abrasion | M | ISO 4649 | 25 | mm³ |
| Compression set at 70h @ 23°C | M | ISO 815 | 16 | % |
| Compression set at 24h @ 70°C | M | ISO 815 | 36 | % |
| Softening range low | E | Huntsman TMA | 180 | °C |
| Softening range high | E | Huntsman TMA | 205 | °C |
M = Injection molded parts to meet DIN & ASTM requirements. Parts tempered for 20 hrs @ 100 °C prior to testing
E = Extruded film cut to ASTM requirements. Parts at room temperature aged prior to testing.